Recipe: Desalination paste

Processing

Step 1: Mix 1 kg of Bentonite (#58900) or 1 kg of Attapulgite (#58903) with 250 g of Arbocel® BC 200 (#59755).
Step 2: Then add approx. 2 liters of demineralized water (#65000) while stirring until a paste-like mass is obtained. This mixture yields approx. 2.5 liters of desalination paste.
Step 3: The desalination paste is applied to a thickness of approx. 5 mm. As it dries, the desalination paste pulls the salt out of the substrate and absorbs it. Repeat this process with new desalination paste until the desired result is achieved (usually three times).
Step 4: Consumption is approx. 5 liters per square meter (per application).
Step 5: Consumption per square meter: 4 liters of demineralized water (#65000), 500 g of Arbocel® BC 200 (#59755), 2 kg of Bentonite (#58900) or Attapulgite (#58903).

Ingredients

1 kg Bentonite (#58900)
Alternative:
Attapulgite (#58903)
250 g Arbocel® BC 200 (#59755)
2 l Water (#65000)
We assume no liability for the processing instructions described above. In any case, we recommend the production and evaluation of sample surfaces.

Product list